Guide
Dye Migration in Screen Printing: Causes and Fixes
Champion Inks

Dye migration in screen printing is when dye from a polyester garment moves into the ink printed on it. Heat from the flash unit, the dryer or a hot stack of shirts sets it off, and it is the reason a white print on a red polyester jersey can come out pink. No ink switches it off completely, but three defenses used together cut the risk: keep the heat at the low end of the ink's cure range, print a bleed-resistant ink or white, and put a grey blocker underneath on fabrics that bleed hard. Then test the exact garment before you run the order.
Dye migration in screen printing: how it happens
Polyester is colored with disperse dyes, which are set into the fiber with heat when the fabric is made. Heat can free some of that dye again. During flashing and curing, dye can leave the fiber and move into the ink film on top of it, and the ink takes on the garment's color: a white goes pink on red or maroon, and a light color picks up the shirt's tint.
Cotton is colored with other dye types that do not move this way, which is why the same white that prints clean on a cotton tee can tint on a polyester one. Anything with polyester in it can bleed: 100% polyester, 50/50s and tri-blends, colored heathers and, above all, sublimated garments, where the design itself is made of dye. Reds and maroons are the usual suspects, and the same style can behave differently from one dye lot to the next.
How to spot it, including the delayed kind
Migration shows up as a color cast that was not in the ink: a pink or peach white on red, a tint on light colors that matches the shirt, or the ghost of a sublimated pattern coming through the print. Before you change inks, rule out show-through, which looks similar but needs a different fix.
| What you see | Likely cause | First thing to try |
|---|---|---|
| The white looks pink or gray before it sees any heat | Show-through: not enough white to hide the shirt | A more opaque white, an underbase, or print-flash-print |
| Clean off the press, tinted after the flash or the dryer | Dye migration driven by heat | Lower the heat, switch to a low-bleed white, add a grey blocker |
| Clean at pack-out, tinted a day or more later | Delayed migration | Low-bleed ink or a blocker, cool prints before stacking, a 24-hour first-piece check |
| A sublimated pattern ghosts through the print | Sublimation dye moving into the ink | A grey blocker under the white and colors |
The delayed kind is the one that costs reprints. Dye can keep moving after the print leaves the dryer, so a shirt that passed inspection can tint hours or days later, sometimes after delivery. That is why the testing routine below ends with a 24-hour check.
Defense 1: control the heat
Heat is the main trigger, so take out every degree and every second the cure does not need. Champion's Athletic Polyester label puts it plainly: "Keep dryer temperatures as low as cure allows to minimize dye migration." In practice:
- Choose a lower-cure ink for bleed-prone polyester. On Champion's labels, the Extreme 270° Low Cure colors and white and the IronBlock LC grey blocker cure at 270–290°F, and the Athletic Polyester colors and Sport White at 280–300°F. Standard lines such as Bleed Resistant and General Purpose list 320–330°F.
- Measure the ink, not the dial. What matters is the temperature the ink film reaches. Profile the dryer with a probe or temperature strips; an infrared gun reads only the surface.
- Flash to a gel and stop. Every flash adds heat to the garment, so flash only until the ink is just dry to the touch, and watch for pallets that heat up over a long run.
- Cure the stack at the right number. When you layer inks, the whole film has to reach the highest cure temperature among them. A low-cure blocker under a standard-cure color still needs the color's temperature, so build heat-sensitive jobs from inks in the same low range.
- Cool before you stack. Lay prints out as they leave the dryer, or put a fan on them: heat trapped in a stack keeps driving dye into the ink.
Lower heat never means undercuring. The target is the low end of the label's range, reached all the way through the ink film.
Defense 2: bleed-resistant inks and whites
Bleed-resistant (low-bleed) inks are formulated to hold back the garment's dye, and the white matters most because it shows the faintest tint. Here is how Champion's labels position each option:
| Ink | Label lists it for | Label cure |
|---|---|---|
| Bleed Resistant (BR) colors | 100% cotton, 50/50 cotton–poly blends, light-colored polyester | 320–330°F |
| BR 5-Star Bright White CQ | 100% cotton, 50/50 cotton–polyester blends, light polyester garments | 320–330°F |
| Sport White | Polyester, athletic wear and moisture-wicking fabrics | 280–300°F |
| Athletic White Fast Flash | 100% polyester, sublimated and performance fabrics | 320–330°F |
| Athletic Polyester colors | Jerseys, team uniforms and performance wear in 100% polyester and stretch fabrics | 280–300°F |
| Extreme 270° Low Cure White and colors | 100% polyester, blends and moisture-wicking fabrics | 270–290°F |
Two details in those labels are worth acting on. First, bleed resistance depends on a full cure: the Sport White label says "Fully cure at 280°F–300°F for optimal bleed resistance," and the Athletic White label ties its "max bleed resistance" to the ink reaching 320–330°F. Second, on dark polyester the BR labels call for a low-bleed white underbase instead of relying on the color alone. The 5-Star label puts it this way: "For dark sublimated polyester, use this as the underbase to boost color vibrancy and resist bleed."
For press technique on a white underbase, including print-flash-print, see how to use Champion white plastisol ink.
Defense 3: a grey blocker underneath
A grey blocker (also written gray blocker) is a high-opacity grey plastisol printed first, under the white and colors, as a barrier between the dyed fabric and the rest of the print. Champion offers two grey blocker underbases:
- IronBlock LC, the lower-temperature option. Its label gives "Final Cure Temperature: 270°F–290°F (132°C–143°C) for complete curing," a 220°F flash for 3–5 seconds, and mesh from 86 to 305 "depending on fabric and ink deposit requirements." It lists polyester, tri-blends, cotton/poly blends and sublimated garments, with white or color plastisol on top.
- Grey Blocker Underbase, which cures at a higher temperature than IronBlock LC, so take its cure range from the container before you set the dryer. Its label gives a 250°F flash for 3–5 seconds and 110–160 mesh for standard prints, and lists dark garments "as an underbase for bright top colors."
A typical sequence is grey blocker, flash to a gel, white underbase where the design needs one, flash, then the colors and a full cure at the temperature the whole stack needs. Choke the blocker art slightly so no grey peeks out at the edges, and do not over-flash it: a blocker cooked hard on press can weaken its bond with the layers above.
Grey blocker vs white underbase: when to use which
Both go down first and both hold back dye, but they do different jobs. A low-bleed white underbase brightens the colors above it and blocks moderate bleed in a single layer. A grey blocker's main job is to stop dye. It costs an extra screen, an extra flash and some extra thickness, so add it when the garment calls for it.
| Situation | Start with |
|---|---|
| Ink darker than the garment | Low-bleed ink and heat control; any dye that moves is hard to see |
| White or light ink on 50/50s, colored heathers or light polyester | A low-bleed white, such as BR 5-Star Bright White CQ or Sport White, as the white or the underbase |
| Bright colors on dark polyester | A low-bleed white underbase under the colors, as the BR labels recommend |
| Sublimated garments, deep reds, maroons or camo on 100% polyester | Grey blocker, then the white, then the colors |
| A low-bleed white that still tinted at the 24-hour check | Add a grey blocker under it |
When the call is close, print both versions on the test garment and compare them after 24 hours.
A testing routine before full production
- Test the exact blank. Same style, same color and, ideally, the same carton or dye lot as the order. Another color of the same style is not a test.
- Print with production settings. Use the same inks, mesh, flash and dryer settings, and measure the temperature the ink film reaches in the dryer.
- Check it twice on day one. Inspect it hot off the dryer and again once it has cooled.
- Check it again at 24 hours. This is the interval on Champion's Athletic Polyester label: "Test the first piece for bleed after 24 hours before running the full order."
- Wash it. Wash and dry the sample the way the end customer will, then look for tint, cracking and fading.
- Write down what passed. Ink, mesh, flash time, belt speed, dryer setting and measured temperature, so the reorder runs the same way.
During the run, set a few pieces aside and look at them again before the order ships.
What not to rely on
- One ink as a guarantee. Garment dyes are not standardized, and no ink blocks every dye on every blank. A label tells you what an ink is built to do; your test tells you what it does on this shirt.
- Undercuring to dodge bleed. Pulling the heat below the ink's cure range trades a tint for prints that crack and wash out. If the garment cannot take the heat an ink needs, change to a lower-cure ink instead.
- A heavier white on its own. Extra white can hide a faint tint at first, but dye that keeps moving can still come through, and a thicker film needs more time in the dryer to cure all the way through.
- Last season's test. Re-test when the blank, color or dye lot changes, even on a familiar style.
If a blank keeps bleeding after you have worked through all three defenses, contact Champion with the garment style and color, the inks, your mesh and your dryer settings.
Shop the inks
- Grey blocker underbase collection: IronBlock LC (270–290°F) and Grey Blocker Underbase
- Bleed Resistant plastisol for blends, with BR 5-Star Bright White CQ for whites and underbases
- Extreme 270° Low Cure inks: colors and a white for heat-sensitive polyester
- Athletic Polyester Plastisol Ink for jerseys and team uniforms
- Not sure which range fits the fabric? Try the ink finder.
Label figures in this guide were checked against Champion's product pages on November 24, 2026. Always follow the label on the container you are printing from.
Frequently asked questions
What causes dye migration in screen printing?
Mostly heat. Polyester is colored with disperse dyes, and the heat of flashing, curing and hot stacking can release them into the ink film above. Sublimated garments, reds and maroons are frequent offenders, but any dyed polyester or poly blend can bleed, and results vary by dye lot. Cotton is colored with other dye types that do not move this way, so the same print can stay clean on cotton and tint on polyester.
Why did my white ink turn pink on a polyester shirt?
If the white was clean after the print stroke and turned pink after the flash, the dryer or a day in the box, dye from the shirt migrated into it. If it looked pink before any heat, the white was simply too thin to hide the shirt. For migration, cure at the low end of the ink's range, switch to a low-bleed white and, on heavy bleeders, print a grey blocker first.
Does low-cure ink stop dye migration?
It lowers the risk; it does not guarantee a clean print. Less heat gives the dye less push, which is why the label on Champion's Extreme 270° White says its low cure "Reduces risk of dye migration, scorching, and garment shrinkage." Some fabrics bleed even at low temperatures, so pair a low-cure ink with a low-bleed white or a grey blocker where needed, and test the exact garment.
When should I use a grey blocker instead of a white underbase?
Use a grey blocker when the garment bleeds hard: sublimated prints, deep reds, maroons or camo on 100% polyester, or any blank where a low-bleed white still tinted at the 24-hour check. Print it first, flash it to a gel, then add the white and colors. On lighter or less aggressive blends, a low-bleed white underbase is often enough on its own, with one less screen and a softer print.
How long after printing can dye migration show up?
It can appear as the shirt leaves the dryer, or hours to days later as dye keeps moving into the ink, sometimes after the order has shipped. That is why Champion's Athletic Polyester label says to test the first piece for bleed after 24 hours before running the full order. Let prints cool before stacking, and recheck a few pieces from the run before delivery.