Guide
How to Cure Plastisol Ink: Flash, Dryer & Heat Press
Champion Inks

To cure plastisol ink, heat the entire ink film, not just its surface, to the full-cure temperature listed for that ink. Flash only to gel each layer between colors, do the full cure in a conveyor dryer (or, on small runs, carefully with a heat press or flash unit), and prove it with a temperature reading taken on the print plus a wash test before the run.
There is no single cure number for every plastisol. Champion’s product pages list full-cure temperatures as low as 270°F for its low-cure polyester inks and 320–330°F for standard cotton inks, so the table below gives each series its own settings.
What “cured” actually means
Plastisol changes in two stages as it heats. First the PVC particles start to absorb the plasticizer and swell, and the ink gels: the surface becomes dry to the touch and can take another layer, but the film is still weak and would crack or wash away. With more heat, the swollen particles fuse into a tough, flexible film that holds onto the fabric. That is the cure, and it has to happen all the way through the deposit. Champion’s All Purpose page says it in one line: “320°F (160°C) – entire ink film must reach temperature.”
The bottom of the ink film, where it meets the fabric, is the last part to get there. The garment soaks up heat, and a thick underbase or a heavy hoodie slows things further, so a print can feel cured on top while the layer underneath is not. That hidden undercure shows up later as cracking, flaking or fading in the wash.
More heat is not automatically better. Too much can scorch or shrink garments and drive dye migration on polyester, and some inks lose their effect: the Fluorescent page warns, “Do not over-cure; excess heat dulls fluorescent pigments.”
Plastisol ink cure temperatures and flash settings by series
These are the flash and full-cure settings on Champion’s product pages. The cure figure is the temperature the whole ink film must reach; the flash figure is the target for gelling the surface between colors.
| Ink | Flash (listed) | Full cure (listed) |
|---|---|---|
| All Purpose | 220–250°F (104–121°C), 3–5 sec | 320°F (160°C) |
| General Purpose colors | 250°F (121°C), 3–5 seconds | 320–330°F (160–165°C) |
| High Opacity | 220–250°F (104–121°C), 3–5 sec | 320–330°F (160–165°C) |
| Bleed Resistant | ~250°F (121°C), 3–5 seconds | 320–330°F (160–165°C) |
| General Purpose White and White Fast Flash | 220–250°F (104–121°C), 3–5 seconds | 320–330°F (160–165°C) |
| Sport colors | 250°F (121°C), 3–5 seconds | 320–330°F (160–165°C) |
| Sport White | 220–250°F, 3–5 seconds | 280–300°F (138–149°C) |
| Athletic Polyester colors | ~210°F (99°C), 3–5 seconds | 280–300°F (137–148°C) |
| Athletic White Fast Flash | 220–250°F (104–121°C), 3–5 sec | 320–330°F (160–165°C) |
| Extreme 270° Low Cure colors and white | 220°F (104°C), 3–5 seconds | 270–290°F (132–143°C) |
| IronBlock LC gray blocker | 220°F (104°C), 3–5 seconds | 270–290°F (132–143°C) |
| Puff | 250°F (121°C), 3–5 seconds between layers | 320–330°F (160–165°C) |
| Glitter, Metallic, Shimmer, Fluorescent, Glow, Reflective | 220–250°F (104–121°C) | 320°F (160°C) |
Two rules: the label on your container outranks any chart, including this one. And when a print stacks inks with different cure ranges, every layer still needs its full cure, so the whole print has to reach the highest cure temperature in the stack: a low-cure blocker under a 320°F top color still has to see 320°F. If an ink you use is not listed here, follow its own specs, or send us your dryer settings and ask.
Flash curing: gel the layer, don’t cure it
The flash exists so the next screen can print on top of a layer without lifting or smearing it, and that only takes a gel. All Purpose says to flash “until surface is dry to the touch,” and Champion’s white plastisol printing guide adds, “Do not fully cure during flash.”
Distance, time and temperature
The listed flash settings describe what the ink needs, not how to set your flash unit. Real flash time depends on the unit’s power, its height above the platen and how hot the platen already is:
- Warm up the flash and the platens before the run, so the first shirts behave like the rest.
- Start from the listed time, then touch a corner of the print lightly. If ink comes off on your finger, add time; if the surface turns hard and rough, or puff starts to rise, cut time or raise the flash.
- Check the ink surface with an infrared thermometer to confirm you are near the listed flash temperature, not well past it.
- Re-check during the run. Platens soak up heat, so a flash time that is right on the first shirt can be too long by the fiftieth.
Some products are built to flash faster: Quick Flash Reducer is “engineered to reduce flash times” and “Specially optimized for BR and GP series plastisol inks,” added at up to 5% by weight.
Signs of over-flashing
- Rough, stacked texture. Champion’s white plastisol guide warns that over-flashing “can cause ink stacking, rough texture, or dye bleed on sensitive fabrics.”
- Poor bonding of the next layer. A base cured hard at the flash gives the next ink less to grip. For puff printed over a base, Champion’s fluorescent puff guide notes that “Over-curing the base layer can create poor bonding and uneven lift.”
- Puff rising early. If puff swells at the flash station, the Puff page’s fix is to “lower the flash temperature or raise the flash height.”
- Dye bleed on polyester. Flash heat counts too; Champion’s stretch plastisol guide warns, “Too much heat during flashing can trigger dye bleed on performance fabrics.”
Conveyor dryers: dwell time matters as much as the setpoint
A conveyor dryer cures with heat over time. The number on the controller is the heater or chamber temperature, not the temperature your ink reaches. What the ink film actually sees depends on the heater setting, its height above the belt, belt speed (which sets the dwell time), the garment’s weight and color, the thickness of the deposit and even how cold the shop is. A heavy hoodie with a thick underbase needs more heat or time than a light tee with one thin color.
Profile the dryer with the jobs you actually run:
- Let the dryer warm up fully before the first test.
- Run a real garment printed with the real deposit, with a temperature strip on the print or a probe riding along on it.
- If the peak falls short of the listed range, slow the belt first to add dwell time, and raise the heat in small steps only if slowing down is not enough. If it overshoots, do the reverse.
- Record what worked for that garment and ink: belt speed, heater setting and height, and the reading.
On polyester, the Athletic Polyester page advises: “Keep dryer temperatures as low as cure allows to minimize dye migration.” Let prints cool before you stack them, especially puff: the fluorescent puff guide warns that “pressing the print while it’s still hot can flatten the puff effect.”
Curing with a flash unit or heat press on small runs
Many small shops start without a conveyor dryer. Both workarounds can cure plastisol on short runs if you verify every setup, but they heat less evenly and leave less margin for error.
Flash unit. Most flash units heat unevenly across their footprint, and leaving a garment under one long enough to cure the full film also heats the platen and can scorch the fabric. Keep the whole print inside the heated area, put temperature strips at the center and the edge of the print, and wash-test a sample before you print the order. For puff, use a dryer: the fluorescent puff guide says, “You must run puff ink through a proper dryer. A flash alone is not a full cure.”
Heat press. Gel the print with a flash first, cover it with a release sheet so ink can’t transfer to the platen, and press with light pressure at the ink’s listed cure temperature. Then confirm with a temperature strip and a wash test. Expect a smoother, flatter surface than a dryer gives, and don’t press puff or high-density prints; the fluorescent puff guide says puff “is not meant to be scraped, ironed, or high-heat pressed after cure.”
How to prove a cure
Measure the ink film, not the dryer air
What matters is the temperature the ink film reached. Temperature strips, heat-sensitive labels that change color at set temperatures, ride through the dryer on the print and record the peak. A thermocouple probe on the print gives a live reading of the same thing. An infrared gun is handy for quick checks, but it reads only the surface at the moment you aim it, so take the reading on the ink itself as the print leaves the heat. Champion’s white plastisol guide says the same: “Use a laser temp gun or probe directly on the print while it’s on the belt.”
Stretch test
Once the print has cooled, stretch it firmly in both directions. A well-cured plastisol print stretches and recovers; the white plastisol guide’s standard is that “The ink should stay smooth with no cracking or lifting.” Cracking usually points to undercure, though a very heavy deposit or an ink not built for stretch can crack even when cured, and a print can pass this test and still fail in the wash. Treat it as a quick screen, not proof.
Wash test
The wash test is the proof. Before the production run, print a sample on the same blank with the same ink, deposit and dryer settings, then wash and dry it several times the way your customer will. Compare it with an unwashed print and look for cracking, flaking, fading or ink lifting at the edges. The white plastisol guide sets the bar: “A good cure stays bright and does not chalk off or fade to gray.” It also suggests a fingernail scratch test: “If ink wipes or powders off, it’s undercured.”
Heat-sensitive fabrics: when to switch to low-cure ink
If you are curing polyester at 320°F or more and fighting pink whites, scorch marks or shrinkage, change the ink system instead of fighting the dryer. Extreme 270° low-cure plastisol lists “Curing Temperature: 270°F–290°F (132°C–143°C) for full cure,” Athletic Polyester Plastisol Ink cures at 280–300°F, and IronBlock LC, a gray blocker underbase, lists “Final Cure Temperature: 270°F–290°F (132°C–143°C) for complete curing.”
Build the whole stack from low-cure inks so the dryer can stay low, then test the first piece and look at it again the next day, because migration can keep developing after printing. The Athletic Polyester page says: “Test the first piece for bleed after 24 hours before running the full order.” For dye-prone polyester, see Champion’s gray blocker underbases.
Shop the inks
- Champion plastisol inks, every series in one place.
- Extreme 270° low-cure plastisol for heat-sensitive polyester.
- White plastisol inks, including fast-flash whites.
Settings on this page are quoted from Champion’s product pages and Learning Center guides on championinks.com, last reviewed November 24, 2026. Specs can change; if the label on the container you are printing differs, follow the label.
Frequently asked questions
What temperature does plastisol ink cure at?
It depends on the ink. Champion lists 320°F (160°C) for All Purpose, 320–330°F (160–165°C) for General Purpose and Sport colors, 280–300°F for Athletic Polyester and Sport White, and 270–290°F for Extreme 270° Low Cure and IronBlock LC. The whole ink film has to reach it.
Can you cure plastisol ink with a heat press?
Yes, on small runs, if you verify it. Gel the print, cover it with a release sheet and press lightly at the ink’s listed cure temperature. Confirm with a temperature strip and a wash test. Don’t press puff or high-density prints.
Can you cure plastisol ink with a heat gun?
Only for tests and one-offs. A heat gun heats a small spot at a time, so it is hard to cure the whole ink film evenly without scorching the garment. For work you sell, use a dryer or a verified heat press.
How long should you flash plastisol between colors?
Only until the surface is dry to the touch. Champion lists 3–5 seconds for most of its inks, such as 220–250°F (104–121°C) for All Purpose, but your flash unit’s power, height and platen heat set the real time. Shorten the flash as platens warm up.
Why does my print crack when I stretch it?
Check for undercure first: the bottom of the ink film may never have reached its cure temperature. Measure it with a temperature strip, then slow the belt or add heat. Very heavy deposits, over-flashed base layers and inks not built for stretch can also crack.