Guide
How to Screen Print on Polyester Without Dye Migration
Champion Inks

To screen print on polyester without dye migration, control the heat and put a barrier between the fabric’s dye and your top colors. Print a low-bleed or low-cure plastisol made for polyester, lay a grey blocker first on dark or sublimated garments, flash each layer only to a gel, and run the dryer no hotter than the inks’ full cure requires. Then check the first piece after 24 hours and wash-test it before you run the order.
Why screen printing on polyester is different
Cotton is usually colored with dyes that stay put when you cure a print. Polyester is colored with disperse dyes, and heat sets them moving: at curing temperatures some of the dye turns to vapor and migrates into whatever sits on the fibers, including your ink. That is dye migration. A white printed on a red jersey goes pink, and light colors drift toward the garment color.
Four more things set polyester apart:
- Migration can keep going. Garments stacked hot hold their heat, so a print that looked clean off the dryer can discolor hours later.
- Synthetics are heat-sensitive. Too much heat can scorch or shrink polyester and leave shiny, glazed patches.
- Performance fabric stretches. Many athletic garments contain spandex, so the ink film has to flex with the fabric or it cracks.
- Sublimated garments are the hardest case. Their graphics are printed with dye designed to move under heat, which is exactly what you are trying to stop.
The polyester toolkit
Choosing a polyester screen printing ink comes down to four kinds of product: low-cure colors, bleed-resistant whites, grey blockers that sit under everything, and flexible inks for garments that stretch. The table compares the label settings of Champion’s polyester-capable inks.
| Champion ink | Made for (label) | Flash (label) | Full cure (label) |
|---|---|---|---|
| Extreme 270° Low Cure colors and white | 100% polyester, blends, moisture-wicking fabrics | 220°F, 3–5 sec | 270°F–290°F |
| Athletic Polyester colors | 100% polyester jerseys and performance wear | ~210°F, 3–5 sec | 280–300°F |
| IronBlock LC grey blocker | Polyester, tri-blends, cotton/poly blends, sublimated garments | 220°F, 3–5 sec | 270°F–290°F |
| Grey Blocker Underbase | Polyester, tri-blends, sublimated fabrics | 250°F, 3–5 sec | 290–310°F |
| Sport White | Polyester, athletic wear, moisture-wicking fabrics | 220°F–250°F, 3–5 sec | 280°F–300°F |
| Athletic White Fast Flash | 100% polyester, sublimated and performance fabrics | 220–250°F, 3–5 sec | 320–330°F |
| Sport colors | 100% polyester, spandex, 50/50 blends and cotton | 250°F, 3–5 sec | 320°F–330°F |
| Bleed Resistant 5-Star Bright White CQ | 100% cotton, 50/50 blends, light polyester | ~250°F, 3–5 sec | 320°F–330°F |
Temperatures are in °F as printed on each live product page; confirm them against your container’s label.
Low-cure inks: Extreme 270° and Athletic Polyester
Extreme 270° low-cure plastisol is the lowest-cure color system in this lineup. In the label’s words: “With a cure temperature as low as 270°F (132°C), it minimizes garment shrinkage and migration.” It is designed for 100% polyester, blends and moisture-wicking fabrics, and labeled bleed resistant on sublimated fabrics. It comes as Extreme 270° colors and a matching white, so a whole print can stay in one low-cure system.
Athletic Polyester Plastisol Ink covers 55 team colors. Its label reads “Low cure (280–300°F) – protects sensitive fabrics from scorching or shrinkage,” and it is listed as bleed resistant on “dark and sublimated polyester.” The label also lists 86–160 mesh for general prints and 200+ for fine detail.
Bleed-resistant whites
Migration shows first in the white, so choose it for the fabric and its cure:
- Extreme 270° Low Cure White: a 270°F–290°F cure and a “Bleed-Resistant Formula.” It is the white for an all-low-cure stack.
- Sport White: a “high-opacity, low-bleed plastisol ink formulated for polyester, athletic wear, and moisture-wicking fabrics,” curing at 280°F–300°F.
- Athletic White Fast Flash: a “high-opacity, low-bleed athletic white” for 100% polyester and sublimated fabrics, with a fast flash for multi-color work. Its label cure is 320–330°F.
- Bleed Resistant 5-Star Bright White CQ: a white for cotton, blends and light polyester whose label adds, “For dark sublimated polyester, use this as the underbase to boost color vibrancy and resist bleed.”
For mesh and flashing technique with whites, see the white plastisol guide.
Grey blockers: IronBlock LC and Grey Blocker Underbase
A grey blocker is printed first, under the white, as a barrier between the fabric’s dye and the rest of the print. Champion’s two grey blocker underbases differ mainly in their cure and flash settings:
- IronBlock LC lists a 270°F–290°F final cure (the same as the Extreme 270° system), a 220°F flash, and mesh from 86 to 305 “depending on fabric and ink deposit requirements.” Its label adds “Top Coats: Compatible with white or color plastisol inks.”
- Grey Blocker Underbase is “Designed for polyester, tri-blends, and sublimated fabrics” and “creates a neutral grey barrier layer.” Its label cure range is 290–310°F, with a 250°F flash.
Print the blocker as an even, complete layer; gaps or a starved deposit let dye through. Colors printed over grey also look different from colors over white, which is why the usual stack on dark polyester is blocker, then white, then colors.
Sport and Stretch for high-movement garments
On garments that stretch hard, the ink film has to move. Sport plastisol lists “100% Polyester (moisture-wicking and sublimated fabrics)” among its substrates, along with spandex and blends. Sport colors list a 320°F–330°F cure, so test carefully on sublimated or heat-sensitive garments, and follow the label’s tip to “Use a bright white underbase for enhanced color brilliance and bleed control on dark garments.” Stretch plastisol is formulated “for Lycra, Spandex, polyester, cotton-poly blends, and performance fabrics.” For press technique on stretch fabric, see the stretch plastisol printing guide.
Low-cure plastisol: what it solves and what it doesn’t
Heat drives migration, so less heat means less of it. Champion’s Athletic Polyester label puts the rule in one line worth taping to the dryer: “Keep dryer temperatures as low as cure allows to minimize dye migration.”
What low cure does not do:
- It does not lower the cure of the other inks in the stack. Every layer has to reach its own full cure, so the layer with the highest cure range sets the dryer. Athletic Polyester colors list 280–300°F, but the Athletic White Fast Flash their listing points to lists 320–330°F, so a print using both has to reach the white’s range. If heat is the problem, build the stack from inks that cure alike: IronBlock LC, Extreme 270° White and Extreme 270° colors all list 270°F–290°F.
- It does not make undercure safe. Low cure is not no cure. The whole ink film still has to reach the label range, or the print will crack, fail a stretch test or wash out.
- It does not rule out bleed. On aggressive sublimated or heavily dyed fabric, low-cure ink lowers the risk; a blocker adds protection, and the 24-hour check confirms the result.
A print sequence for dark polyester
Use this conservative starting sequence on dark or sublimated polyester. Follow each product’s label for flash and cure, and adjust from your tests.
- Load without stretching. Use a light coat of pallet adhesive and lay the garment flat. Fabric stretched on the pallet relaxes after printing and distorts the image.
- Print the grey blocker, IronBlock LC or Grey Blocker Underbase, as an even layer, choked slightly inside the white so the grey never shows at the edges.
- Flash to a gel, not a cure. Dry to the touch is enough; IronBlock LC lists 220°F for 3–5 seconds. Extra flash heat starts the dye moving before the print is finished, and pallets warm up as a run goes on, so recheck flash times.
- Print the white: a low-bleed polyester white whose cure matches the stack, such as Extreme 270° Low Cure White.
- Flash the white to a gel at its label setting (220°F for 3–5 seconds for Extreme 270° White), just long enough to stop the next screens picking it up.
- Print the colors wet-on-wet where you can, in a polyester series such as Extreme 270° or Athletic Polyester.
- Cure every layer to its label range, measured in the ink film. The ink with the highest range sets the target.
- Cool before stacking. Spread garments out until they are cool to the touch; a hot stack keeps migration going.
On white and light-colored polyester you can often skip the blocker and print low-bleed colors directly. On less aggressive dark polyester, a bleed-resistant white underbase may be enough: Champion’s Bleed Resistant colors label suggests “a white blocker underbase (e.g., 5-Star Bright White)” for dark polyester. Let the 24-hour check decide whether a job needs the grey.
Dial in the dryer
- Measure the ink, not the air. The dryer set point is the chamber temperature, not the print’s. Use temperature strips, a probe or a data logger on a test shirt, and confirm the whole ink film reaches the label range.
- Hit the range; don’t overshoot it. Extra heat does not make a polyester print tougher. It drives more dye into the ink and can scorch, shrink or glaze the fabric, so aim inside the label range, not above it.
- Balance belt speed and heat. A thick stack of blocker, white and colors takes longer to heat through than one color, and a slower belt at moderate heat cures it more gently than a fast belt with the heaters turned up.
Test before the run
Champion’s Athletic Polyester label gives a simple protocol: “Test the first piece for bleed after 24 hours before running the full order.” In practice:
- Print and cure a first piece on the exact blank, same style and color, at production settings.
- Let it cool and set it aside for 24 hours. Keep a reference for comparison, such as the same white printed on a cotton shirt.
- Compare the white and light colors with the reference in good light. A pink, grey or green cast means dye is moving.
- Stretch the print. If it cracks, suspect undercure first, or an ink that is not made to stretch.
- Wash and dry the piece the way the garment’s care label allows, then check color, cracking and adhesion again.
If the first piece bleeds, change one thing at a time: add or upgrade the blocker, move to a lower-cure stack, shorten the flash dwell, cool garments faster, or try a different blank. Record the settings that pass.
Nylon and coated fabrics
Nylon jackets, bags and coated fabrics are a different job, where adhesion matters as much as bleed. The label on Champion’s Nylon White Plastisol Ink marks catalyst mixing as “Required for Nylon,” with a limited pot life once catalyzed, so ask Champion about the catalyst and mixing before you plan a nylon job.
Shop the inks
- Extreme 270° low-cure plastisol in colors and white.
- Athletic Polyester Plastisol Ink in 55 team colors.
- Grey blocker underbases: IronBlock LC and Grey Blocker Underbase.
- Sport plastisol and Stretch plastisol for high-movement garments.
- Bleed Resistant plastisol for blends and light polyester.
- Not sure which series fits your blank? Try the ink finder for polyester and blends.
Label settings quoted in this guide were checked against Champion’s live product pages on November 24, 2026. Labels can change, so the container label is the final word.
Frequently asked questions
Can you screen print plastisol on polyester?
Yes, with inks made for it. Plastisol made for cotton often cures hotter than polyester likes, which can draw the fabric’s dye into the print. Choose a low-bleed or low-cure series labeled for polyester, add a grey blocker on dark or sublimated garments, flash only to a gel, and keep the dryer no hotter than full cure requires. Test the first piece before the run.
What temperature should I cure ink on polyester?
Use the full-cure range on each ink’s label, measured in the ink film, and no hotter. Champion’s labels differ: Extreme 270° lists 270°F–290°F, Athletic Polyester colors 280–300°F, and Sport colors 320°F–330°F. When you stack inks, the layer with the highest cure range sets the dryer, so build the stack from low-cure inks if heat is the problem.
What is low-cure plastisol ink?
Low-cure plastisol fully cures at a lower temperature than standard plastisol, cutting the heat that drives dye migration, scorching and shrinkage. Champion’s Extreme 270° series lists a cure as low as 270°F (132°C). Low cure is not no cure, though: the whole ink film still has to reach the label range, or the print will crack and wash out.
Why do prints on polyester change color a day later?
That is dye migration. Heat from flashing and curing turns some of the fabric’s disperse dye into vapor that moves into the ink, and it can keep moving while garments sit warm in a stack. A white on a red jersey turns pink. That is why Champion’s Athletic Polyester label says to check the first piece for bleed after 24 hours.
Do I need a grey blocker on polyester shirts?
Not on every shirt. White and light-colored polyester often prints fine with a low-bleed ink and a careful cure. On dark, red, heavily dyed and sublimated garments, a grey blocker earns its screen: it goes down first, under the white, as a barrier against the fabric’s dye. If the 24-hour check shows bleed, add one.