Guide
Screen Printing Mesh Count Guide by Ink Type
Champion Inks

Screen printing mesh count is the number of threads per inch in the screen fabric. Lower counts have larger openings and put down more ink; higher counts put down less ink and hold finer detail. For most plastisol solids, Champion’s product pages start at 110–160 mesh, detail and halftones move to 200 and up, glitter needs an open 25–40, and four color process runs 230–305.
The tables below collect the mesh ranges listed on Champion’s product pages for more than 30 inks and bases, from everyday plastisol to glitter and water-based inks, plus a note on solvent inks, with the reason each page gives where it gives one. Treat them as starting points, not universal rules: thread diameter, tension and stencil thickness all change what a given count actually prints.
What mesh count controls
- Deposit. Bigger openings let more ink through, which is why underbases, puff and particle inks use lower counts.
- Detail. Fine lines and halftone dots need small openings, with threads close enough together to support them.
- Hand. A thinner deposit feels softer. Champion’s Extender Base page puts it simply: “use higher mesh for softer, thinner prints.”
- Opacity. More ink covers better on dark garments. The Soft Hand Base page says to “use lower mesh for higher opacity.”
Mesh count is not the whole story. The same count can be woven from thicker or thinner thread, and thinner thread leaves more open area, so it passes more ink. Tension matters too: a tight, evenly tensioned screen snaps off the shirt cleanly and prints sharper with less squeegee pressure, while a slack one smears detail. Counts are given in threads per inch in the US and threads per centimeter (“T”) in Europe; divide by about 2.54 to convert. Champion’s solvent ink pages give both, for example “230–280 (92T–112T/cm).”
Screen printing mesh count chart by ink
Every range below is quoted from the product’s page on championinks.com. Where a page explains its range, the reason is included, because it tells you which way to adjust.
Everyday plastisol for cotton and blends
| Ink | Listed mesh |
|---|---|
| All Purpose | 110–160 for solids; 200–230 for detail and halftones |
| General Purpose | 110–160 for standard prints; 200+ for fine detail |
| High Opacity | 110–160 for solids / underbase; 200–230 for detail |
| Bleed Resistant | 110–160 for standard prints; 200+ for fine detail |
| General Purpose White Fast Flash | 110–160 for solid whites; 200+ for fine details |
| Bleed Resistant 5-Star Bright White CQ | 110–160 for opacity; 200+ for finer detail |
| Extender Base | 110–200+ (use higher mesh for softer, thinner prints) |
Polyester, athletic and blockers
| Ink | Listed mesh |
|---|---|
| Athletic Polyester | 86–160 for general prints; 200+ for fine detail |
| Athletic White Fast Flash | 110–160 for coverage; 200+ for finer detail |
| Sport | 110–230 depending on desired ink deposit |
| Stretch | 110–230 for balanced deposit and detail |
| Extreme 270° Low Cure | 110–160 for standard prints; 200+ for fine details |
| Nylon White | 110–160 for coverage; 200+ for finer detail |
| IronBlock LC gray blocker | 86–305 depending on fabric and ink deposit requirements |
| Grey Blocker Underbase | 110–160 for standard prints; 200+ for fine details |
Specialty effects
| Ink | Listed mesh |
|---|---|
| Glitter | 25–40 (glitter flake needs a large opening) |
| Reflective | 60–86 (beads need an open mesh) |
| Glow in the Dark | 60–110 (heavier deposit = longer glow) |
| Foil Adhesive Plastisol Base | 60–110 for optimal adhesive deposit |
| Puff | 86–110 for maximum puff; 160–200 for finer detail and a lower rise |
| Puff White | 110 recommended |
| Metallic | 86–125 (open mesh lets the flake through) |
| Overprint Clear Gel | 86–160 for thicker, raised gloss; 200+ for finer gloss effects |
| Shimmer | 110–156 |
| Fluorescent | 110–156 |
Process, transfer and water-based inks
| Ink | Listed mesh |
|---|---|
| Four Color Process plastisol | 230–305 (higher mesh for finer line counts) |
| Four Color Process water-based set | 230–305 for sharp halftones and fine details |
| Transfer Plastisol | 110–230 |
| Water-Based Textile | 156–230 depending on coverage vs detail |
| Water-Based Fluorescent | 156–230+ for standard graphics; lower mesh for a heavier neon deposit |
Solvent inks for plastics and signs
Champion’s solvent series pages (10000, 20000, 30000, 40000, 43000, 66000 and 76000) list 230–280 (92T–112T/cm) mesh, while the 80000 Coroplast ink lists “200–305 for fine detail / 110–160 for bold prints.” Solvent inks also need a stencil that solvents won’t break down; the Multi-Vac 10000 page recommends “Solvent-resistant films or photo emulsions.”
Matching mesh to the job
Underbases and solid whites
An underbase has one job: lay down enough opaque ink to hide the garment. The High Opacity Plastisol Ink page specifies “110–160 for solids / underbase,” General Purpose White Fast Flash says “110–160 for solid whites,” and Champion’s white plastisol printing guide notes that for underbase and solid white prints on dark garments, “a lower mesh (around 110) is common.” Going finer for a smoother hand is fine as long as you don’t starve the print; the same guide warns, “You still need a solid ink film or the print will look gray and wash out dull.” Many shops print, flash and print again rather than forcing more ink through in one stroke.
Fine detail and halftones
Detail needs small openings and a thin, even stencil. Champion’s core pages move to 200–230 for “detail and halftones” (All Purpose), and the Four Color Process Plastisol Ink page runs “230–305 (higher mesh for finer line counts).” A common starting point is a mesh count roughly four to five times the halftone line count (lines per inch); sources disagree on the exact ratio, so test with your own art. The same page adds a press tip that matters as much as the mesh: “Print wet-on-wet with minimal off-contact for crisp dot registration.”
Flake, bead and phosphor inks
Glitter flake, reflective glass beads and glow pigment are particles, and particles need openings big enough to pass through. Champion’s product pages explain each range in their own words. Glitter Plastisol Ink takes an “Open mesh: 25–40” because “glitter flake needs a large opening.” Reflective takes 60–86 because “beads need an open mesh,” Metallic runs 86–125 because “open mesh lets the flake through,” and Glow uses 60–110 because “heavier deposit = longer glow.”
Shimmer is the exception: it uses fine pearlescent pigment and “Prints like regular plastisol – standard mesh, no special tooling,” at 110–156. Puff inks also want low counts, for height rather than particle size: the Puff page lists “86–110 for maximum puff.” You’ll find most of these in Champion’s specialty plastisol inks.
Water-based inks
Champion lists finer mesh for its water-based inks than for plastisol solids, and a soft, breathable print is often the goal. The Water-Based Textile Ink lists “156–230 depending on coverage vs detail,” and the Water-Based Fluorescent page adds “lower mesh for a heavier neon deposit.” The bigger issue with water-based ink is drying in the screen. The fluorescent page’s advice is to “Keep screens flooded to prevent ink drying in the mesh,” and the textile page calls for a “Water-resistant emulsion suitable for water-based inks.” For long runs, Champion’s water-based retarder is made to “extend open time” at “approximately 1–2% by weight.” Browse Champion’s water-based inks.
Stencil thickness matters as much as mesh
The stencil, the emulsion or capillary film that blocks the mesh where you don’t want ink, adds its own thickness on the print side of the screen. Printers call that added thickness emulsion over mesh, or EOM. A thicker stencil works like a deeper well and deposits more ink; a thinner one lays down less ink and holds fine dots better. Champion’s product pages pair stencils with inks accordingly:
- Glitter: “Use a thick stencil (high-build emulsion or capillary film) for the brightest sparkle.”
- Puff: “Thick stencil or multiple emulsion coats.”
- Halftones: “Use a thin, smooth stencil (low EOM) for the cleanest halftones.”
- Solvent inks: a solvent-resistant film or emulsion, per the Multi-Vac 10000 page.
Mesh and stencil work as a pair. An open mesh with a thin stencil can still starve a glitter print, and a fine mesh with a heavy stencil will fight you on halftones.
Squeegee pairings from Champion’s specs
Most of Champion’s plastisol pages call for a 65–75 durometer squeegee, the middle of the range. Softer blades and slower strokes push more ink; harder, sharper blades shear the ink cleanly and lay down a thinner, crisper film. The specialty pages move off the middle for exactly that reason.
| Ink | Listed squeegee |
|---|---|
| All Purpose (typical core plastisol) | 65–75 durometer, medium pressure |
| Glitter | 60–70 durometer, slow stroke, firm flood |
| Metallic | 60–70 durometer, medium pressure |
| IronBlock LC | 60–70 durometer, medium pressure |
| Reflective | 65–70 durometer, single stroke |
| Glow in the Dark | 65–70 durometer |
| Four Color Process plastisol | 70–75 durometer, sharp edge, light pressure |
| Water-Based Textile | 70–75 durometer |
| 80000 Coroplast solvent | 70–80 durometer |
Glow ink is hard on tools, so its page also advises: “Use a stainless squeegee holder and clean screens promptly – glow pigment is abrasive.”
Common mesh mistakes
- Flake ink through fine mesh. Glitter, metallic and reflective particles can’t pass through openings that are too small, so the screen clogs and the print looks starved. Use the open ranges on those pages.
- Halftones on coarse mesh. Small dots need threads to sit on. On too coarse a mesh, the smallest dots fall through or fill in and fine detail is lost. Move up to the 230–305 range the process inks list.
- A thin white on a dark shirt. Too fine a mesh, or too thin a stencil, leaves a white that looks gray. Drop back to the 110–160 underbase range or print, flash and print.
- Reducing ink to force it through. Thinning ink so it passes a fine mesh costs coverage; the All Purpose page warns, “over-reducing lowers opacity.” Change the mesh instead. Some inks shouldn’t be reduced at all: the Reflective page says, “Stir gently to keep beads suspended; do not reduce.”
- The wrong stencil for the ink system. Water-based inks need a water-resistant stencil and solvent inks a solvent-resistant one, or the stencil can break down mid-run.
Shop the inks
- Specialty plastisol inks: glitter, metallic, shimmer, glow, reflective, puff and four color process.
- Glitter Plastisol Ink for open-mesh sparkle.
- Four Color Process Plastisol Ink for halftones on high-count mesh.
- High Opacity Plastisol Ink for underbases and solids on dark cotton.
- Not sure which ink you need? Match an ink to your fabric.
Mesh, stencil and squeegee settings on this page are quoted from Champion’s product pages and Learning Center guides on championinks.com, last reviewed November 24, 2026. Specs can change; if the label on the container you are printing differs, follow the label.
Frequently asked questions
What mesh count should I use for plastisol ink?
For most plastisol solids, start at 110–160 mesh and move to 200 or higher for fine detail. That is what Champion’s core plastisol pages recommend; All Purpose, for example, lists 110–160 for solids and 200–230 for detail and halftones. Specialty plastisols differ, from 25–40 for glitter to 230–305 for four color process, so check each ink’s specs.
What mesh count is best for a white underbase?
Usually 110–160. Champion’s High Opacity page lists 110–160 for solids and underbase, and Champion’s white plastisol guide notes that around 110 is common for underbase and solid whites on dark garments. Go finer only if you can still lay down a solid ink film, because a starved underbase makes the whole print look gray.
What mesh count do you use for glitter ink?
A very open one. Champion’s Glitter Plastisol page calls for an open 25–40 mesh because the flake needs a large opening, plus a thick stencil, a 60–70 durometer squeegee and a slow stroke with a firm flood. A finer mesh traps flake in the screen and gives a weak, patchy sparkle.
What mesh count is used for halftones and four-color process?
High counts. Champion’s Four Color Process pages list 230–305, with the higher end for finer line counts, and its core plastisol pages use 200–230 for detail and halftones. A common starting point is a mesh count about four to five times the halftone line count, but sources vary, so test with your own art, stencil and ink.
Does a higher mesh count make a softer print?
Generally, yes. A higher count passes less ink, so the cured film is thinner and feels softer; Champion’s Extender Base page says to use higher mesh for softer, thinner prints. The trade-off is opacity: thinner deposits cover less on dark garments, which is why underbases and solid whites usually stay in the 110–160 range.