Guide
Screen Printing on Nylon: Jackets, Bags and Catalysts
Champion Inks

Screen printing on nylon works when you choose one of two routes and prove adhesion before the run. Route one is a plastisol made for nylon, mixed with its catalyst and cured to the label. Route two is an air-dry solvent ink formulated for nylon, which needs no cure oven. Nylon is slick, often coated and sensitive to heat, so ordinary cotton plastisol may scratch or peel off a jacket or bag. Below are both routes with the settings from Champion's product pages, plus the prep and testing steps that keep orders from coming back.
Why screen printing on nylon is tricky
Nylon (polyamide) gives ink very little to grab. Three things work against you on windbreakers, coach jackets, bags and other nylon goods:
- A smooth, tight surface. Nylon shell fabrics are tightly woven and often finished smooth, so ink sits on top of the fibers instead of locking into them the way it does on cotton.
- Coatings and finishes. Many nylon goods carry a water-repellent finish or a coating. The ink has to bond to that layer, and some finishes are designed to shed liquids.
- Heat. Nylon shells, coatings, linings and insulation can scorch, glaze, pucker or shrink if you run them too hot or too long. You need a full cure on the ink without damaging the garment.
That makes nylon a test-first job. The ink matters, but so do the exact garment, its finish and your dryer.
Route 1: catalyzed nylon plastisol
Champion's Nylon White Plastisol Ink is a BR Series white that its product page describes as "a high-opacity, bleed-resistant plastisol formulated for nylon, polyester, coated fabrics, and blends." Its ideal substrates start with "100% Nylon & Coated Nylon" and also include 100% polyester, cotton/polyester blends and 100% cotton, and the page names athletic gear, jackets, bags and performance wear as typical work.
On nylon, the catalyst is not optional. The page's mixing section is headed "Catalyst Mixing (Required for Nylon)."
Mixing the catalyst and pot life
- Weigh it. The page says: "Use Champion Nylon Catalyst: Add 15–20% by weight to the ink." Tare a clean cup on a scale, weigh the ink, then add catalyst at 15–20% of that weight. For 1,000 g of ink, that is 150–200 g of catalyst.
- Mix it completely. The page asks you to "Stir thoroughly to ensure uniform activation and performance." Scrape the sides and bottom of the cup so no unmixed ink reaches the screen.
- Mix only what the job needs. In the page's words: "Pot life is limited once catalyzed; unused mixed ink will harden." No working time is given, so mix small batches, write the mixing time on the cup and keep catalyzed ink apart from your uncatalyzed stock.
- Clean up before it sets. The page warns: "Do not leave catalyzed ink exposed to air—hardened ink cannot be reused." Clear screens, squeegees and tools promptly.
- Protect yourself. The page calls for gloves, safety glasses and proper ventilation during printing and curing. Read the Safety Data Sheets for the ink and the catalyst before you mix.
Uncatalyzed ink keeps far longer: the page lists "Shelf Life: 12 months (un-catalyzed, sealed)," stored at 65–90°F (18–32°C) away from direct sunlight. For the catalyst itself, and for its working time at the batch size you mix, ask Champion about nylon catalyst.
Printing, curing and post-press
The Nylon White product page gives these settings:
| Step | Nylon White product page |
|---|---|
| Mesh | 110–160 for coverage; 200+ for finer detail |
| Squeegee | 65–75 durometer, sharp edge; medium flood with a firm print stroke |
| Flash | 250°F (121°C) for 3–5 seconds |
| Cure | 320–330°F (160–165°C) for 40–50 seconds for full fusion |
| Post-press | A quick double heat press is recommended to enhance adhesion and durability |
Plastisol cures when the ink film itself reaches temperature, so check the print with a probe or temperature strips rather than trusting the dryer setting alone. Then check the garment: run one test piece at the listed cure and inspect the shell, the lining and any coating for scorching, shine or puckering before you commit the order. The page doesn't list press settings for the post-press, so use a non-stick cover sheet, test on a sample first and ask Champion if you need a starting point.
Need a color other than white? CHAMP-MIX™ Custom Color Match lists Nylon Plastisol as one of its ink series, so you can order custom-matched nylon plastisol colors from your color code by the quart, gallon or 5-gallon pail. Confirm the catalyst requirement for your matched color when you order.
Route 2: air-dry solvent inks for nylon goods
Solvent inks dry as the solvent evaporates, with no cure oven. That makes them a practical choice for nylon items that won't run down a dryer belt or can't take plastisol cure temperatures: bags, cases, straps, panels and other hard-to-heat goods. Two Champion air-dry series list nylon on their product pages.
| Product page spec | 66000 Series | 76000 Series |
|---|---|---|
| Ink type | Air-dry solvent-based polyurethane | Solvent-based polyester, air dry |
| Substrates | Nylon, polyester, polyurethane, rubber, leather, cotton, denim, canvas | Treated or untreated polyester, PET/PET-G, nylon, polyester-coated metal, melamine |
| Finish | Smooth, flexible, high-gloss | Glossy, scuff-resistant |
| Drying | Air dry 30 min, or jet dry 20–30 sec at 135–180°F | Air dry 30 min, or jet dry 20–30 sec at 135–180°F |
| Mesh | 230–280 monofilament polyester | 230–280 monofilament polyester |
| Stencil | Solvent-resistant emulsion | Solvent-resistant emulsion |
66000 Series for flexible nylon goods. The 66000 Series Polyurethane Screen Printing Ink leads with "Exceptional flexibility" and is "engineered for polyurethane, nylon, polyester, leather, rubber, and other demanding substrates." Its page adds: "High Resistance – Endures dry cleaning, heat, and environmental exposure for extended durability." For slick, hard-to-wet nylon, Champion's OPTI-922 Biting & Retarder is developed for 66000 Series inks. It is "engineered to enhance adhesion, flow, and durability on the most demanding substrates such as polyurethane (PU), nylon, polyester, latex, and leather," at 3–5% by weight. Custom colors are possible here too: Solvent 66000 is one of the ink series on CHAMP-MIX™ Custom Color Match.
76000 Series for nylon hard goods. The 76000 Series polyester solvent ink is "formulated for treated and untreated polyester, PET, PET-G, nylon, and coated metal." Its page names P-O-P displays, indoor signage and industrial printing as its uses and doesn't mention garments. Reach for it on nylon parts and panels, and test carefully before using it on anything that flexes or gets washed.
Working with solvent inks on nylon:
- Match the screen to the ink. Use the listed 230–280 mesh and a solvent-resistant emulsion. A stencil made only for plastisol may not hold up to solvent.
- Adjust only with the series' own additives, by weight. The 66000 page lists T-974 Retarder at 3–5% to extend open time and T-976 Thinner at 5–10% to reduce viscosity; the 76000 page lists its own T-630 Thinner and T-631 Retarder. Champion's solvent reducers and retarders range includes series-specific products such as OPTI-974 Slow Thinner / Retarder for the 66000 Series and OPTI-631 Retarder for the 76000 Series.
- Work safely. Both pages call for gloves, safety glasses and protective clothing plus good ventilation, and both point you to the Safety Data Sheet before handling.
- Let it dry fully. Give prints their full drying time before you stack, pack or test them.
Prep and hold-down
- Read the content label. Confirm the shell is nylon and note any coating or water-repellent finish. Plenty of jackets that feel like nylon are polyester; for dark or heavily dyed polyester, the Nylon White page recommends Champion 5-Star Bright White as an underbase.
- Print the item as supplied. Don't try to strip a factory finish. Keep the print area free of lint, dust and hand oils, and test whether your ink bonds to the fabric as it comes.
- Hold it flat. Slick nylon slides. Use platen adhesive and a platen that fits inside the jacket so the print area sits flat without being stretched. Move zipper pulls, snaps, drawcords and pocket edges out of the squeegee path, and make sure seams don't put a ridge under the image.
- Set off-contact. Light nylon can lift with the screen. Adhesive plus enough off-contact gives a clean release and sharp edges.
- Protect the lining. On lined or insulated jackets, flash and dryer heat pass through the shell into the lining. Keep plastisol flashes to the listed 3–5 seconds and check the inside of your test piece for marks.
Test adhesion before the run
Both solvent product pages make testing part of the job. The 66000 page says "Pre-Test: Verify adhesion and flexibility on target substrate before production," and the 76000 page says "Pre-Test: Always test for adhesion and durability prior to production." Treat catalyzed plastisol the same way, and build the test into your quote, not into the run:
- Print a sample on the exact item, same color and lot, with the ink mix, mesh, flash and cure or dry settings you'll use in production.
- Let it cure or dry completely and cool to room temperature before you judge it. Solvent prints can keep gaining adhesion after they feel dry, so retest them the next day.
- Scratch test: drag a fingernail firmly across the edges of the print. Ink that lifts or flakes isn't bonded.
- Tape test: press strong tape over the print, rub it down and pull it off fast. Ink on the tape means poor adhesion.
- Flex test: fold, crumple and stretch the print area, then look for cracks or lifting edges.
- Wash test for garments: wash and dry the sample the way the end customer will, then repeat the scratch test.
- Write down the ink, catalyst percentage, mesh, flash and cure or dry settings, plus the garment style and lot, so you can repeat a passing result.
If a coated or water-repellent item fails on both routes, it may not be a good candidate for screen printing. Find that out on one sample, not on the whole order.
Shop the inks
- Champion Nylon White Plastisol Ink for nylon and coated nylon, used with Champion Nylon Catalyst.
- CHAMP-MIX™ Custom Color Match in the Nylon Plastisol or Solvent 66000 series.
- 66000 Series polyurethane ink for flexible nylon, polyurethane, rubber and leather goods.
- 76000 Series polyester and nylon ink for nylon, polyester, PET and coated-metal hard goods.
- Contact Champion for Nylon Catalyst and help dialing in a new substrate.
Specs in this guide were checked against Champion’s live product pages on November 24, 2026. If the label on your container differs, follow the label.
Frequently asked questions
Can you screen print plastisol on nylon?
Yes, with a plastisol made for nylon and its catalyst. Champion's Nylon White Plastisol Ink lists "100% Nylon & Coated Nylon" among its substrates, and its product page marks catalyst mixing as required for nylon: Champion Nylon Catalyst at 15–20% by weight. Ordinary plastisol without a bonding catalyst may scratch or peel off slick nylon, so print a sample and run scratch and wash tests before production.
Why do you need a catalyst to print on nylon?
Nylon is smooth, tightly woven and often coated, so plastisol sits on the surface with little to grip. The catalyst activates the ink for a stronger bond; Champion's product page says to "Stir thoroughly to ensure uniform activation and performance." The page also recommends a quick double heat press after curing to enhance adhesion and durability. Without the catalyst, the print is more likely to fail a scratch or wash test.
How long does catalyzed nylon ink last once mixed?
Champion's product page gives no fixed time. It says "Pot life is limited once catalyzed; unused mixed ink will harden," and that hardened ink cannot be reused. Mix only what the job needs, write the mixing time on the cup and clean screens and tools before the ink sets. Sealed, uncatalyzed ink has a 12-month shelf life. Ask Champion for working time at your batch size and shop conditions.
Can you screen print on waterproof nylon jackets?
It can work, but test first. Water-repellent finishes and coatings are made to shed liquids, and the ink has to bond to that surface. Champion's Nylon White lists coated nylon as a substrate, used with its catalyst. Print one sample on the exact jacket, cure it to spec, then run scratch, flex and wash tests. If the finish rejects the ink, you want to learn that on one jacket, not on the whole order.
What cure temperature does nylon ink need?
It depends on the ink. Champion's Nylon White Plastisol cures at 320–330°F (160–165°C) for 40–50 seconds for full fusion, after a flash of 250°F (121°C) for 3–5 seconds, and the page recommends a quick double heat press afterward. The 66000 and 76000 solvent series don't heat-cure: they air dry in 30 minutes or jet dry in 20–30 seconds at 135–180°F.