Guide
Screen Printing Troubleshooting: Cracking, Washout & More
Champion Inks

Screen printing troubleshooting goes faster once you know that most problems trace back to a short list of causes. Cracking and washout usually mean the ink film never reached its full cure temperature. Pinholes start in the stencil. Ghosting comes from something moving, or from ink building up under the screen. A white that turns pink on polyester is dye migration. Find your symptom below, run the quick check, and fix the cause, not just the shirt in front of you.
Start with cure
Plastisol doesn't air-dry; it cures. Heat first gels the ink, then fuses it into a solid, flexible film. A print that has only gelled can look finished and feel dry, then crack on a stretch or fade in the first few washes. That's why cure comes first here: an undercured ink film is the most common cause of both cracking and washout.
Cure is a temperature the ink film reaches, not a number on the dryer. Champion's All Purpose label says it plainly: "320°F (160°C) – entire ink film must reach temperature." The target changes by series. General Purpose plastisol cures at 320–330°F, Sport White at 280–300°F and the Extreme 270° Low Cure inks at 270–290°F, so always use the range on the container in hand. (We checked the label specs on this page on November 24, 2026.)
- Measure the ink film, not the dryer air. A thermocouple probe or a temperature strip that rides through the dryer with the print tells you far more than the dryer's set point. An infrared gun reads only the surface at one moment, so treat it as a rough check.
- Give heavy deposits more time. The underside of a thick print heats last. Adding dwell time with a slower belt is often safer than turning up the heat, especially on polyester.
- Prove it before the run. Stretch a cured, cooled print, then wash a sample. A stretch test alone doesn't prove a full cure; the wash test is the one that counts.
Cracking after washing or stretching
Likely causes: an undercured ink film; a heavy deposit whose underside never reached temperature; or a standard plastisol printed on a stretch fabric.
Quick check: Measure the ink-film temperature on the next print. Stretch a fresh, cooled print in both directions. Cracks that open across the image point to undercure, or to an ink that wasn't made to stretch with the fabric.
Fix:
- Bring the entire ink film into the label's cure range, adding dwell time before you add heat.
- Lay down only as much ink as the design needs, using the mesh range on the label.
- On Lycra, spandex and compression wear, use a stretch ink or a stretch additive, and still verify the cure. Champion's Stretch Plastisol label says: "Verify complete cure to ensure elasticity and prevent cracking." For settings, see our stretch plastisol guide for performance wear.
Ink washing out or fading
Likely causes: undercure again, a deposit too thin to hold up, or over-reduced ink.
Quick check: Wash-test a sample from the run and look up the reducer ratio on the job ticket. A fingernail scratch helps too; as Champion's white plastisol guide puts it, "If ink wipes or powders off, it's undercured."
Fix: Cure the full ink film to the label's range. Print on the label's mesh with a consistent stroke so enough ink reaches the garment. Respect the reduction limit; Champion's All Purpose label says, "Do not add more than 5% reducer; over-reducing lowers opacity." With water-based ink, cure only after the water has gone: Champion's water-based label says to fully cure "only after all moisture has driven off."
Pinholes
Pinholes are tiny open spots in the stencil that print as dots where no ink should be. They are a screen-room problem, not an ink problem. The usual causes:
- Mesh that wasn't fully degreased, so the emulsion pulls away and leaves gaps.
- Dust or lint on the mesh, in the emulsion, on the film positive or on the exposure glass.
- Air bubbles in the emulsion, or a coat that went on unevenly.
- Underexposure, which leaves a soft stencil that breaks down on press.
- Coating or exposing a screen that isn't completely dry.
Fix: Degrease every screen before coating. Coat and dry in a clean, dark, dust-free space. Keep the glass and film positives clean. Run an exposure test for your emulsion and light source instead of guessing. Before a screen goes on press, check it on a light table, find any pinholes and block them out.
Ghosting and double images
A faint second image beside the main print almost always means something moved, or that ink is building up where it shouldn't.
- Screen or platen movement: loose clamps, a loose frame or low mesh tension can let the image shift between strokes. Tighten everything and check tension.
- Garment shift: a shirt that slides on the platen prints twice. Use pallet adhesive and load the garment flat.
- Off-contact: with too little off-contact, the mesh drags across the print instead of peeling cleanly away from it. Set enough gap for the screen to lift right behind the squeegee.
- Ink under the screen: ink on the underside of the screen transfers to the next shirt. Wipe the underside regularly. When you flash an underbase, flash it until it is dry to the touch, as Champion's flash specs say; an under-flashed layer gets picked up by the next screen.
An old image you can still see in a reclaimed screen is a different problem: a stain or residue left in the mesh. Deal with it in the screen room, not on press.
Whites turning pink or changing color on polyester
This is dye migration. Polyester is dyed with dyes that can turn to gas under heat and move into the ink. A white turns pink on a red shirt or gray on a black one, sometimes in the dryer and sometimes hours later.
Quick check: Hold the first printed piece for a day. Champion's Athletic Polyester label says: "Test the first piece for bleed after 24 hours before running the full order."
Fix:
- Lower the heat. Use a low-cure ink, and as the same label puts it, "Keep dryer temperatures as low as cure allows to minimize dye migration." Champion's Extreme 270° Low Cure series cures at 270–290°F.
- Switch to a low-bleed white made for polyester.
- Print a grey blocker first on dark or sublimated polyester, flash it, then print the white or colors over it. Champion's grey blocker underbases include IronBlock LC, which cures at 270–290°F and lists white or color plastisol top coats as compatible.
- Let prints cool before you stack them.
A low-cure, low-bleed system reduces the risk; it doesn't remove it. Always test the actual garment.
Dull or gray-looking whites
Likely causes: too little ink on the shirt, an underbase that didn't cover, undercure, over-reduction or, on polyester, dye migration.
Fix: Burn underbase and solid-white screens on the label's solids mesh; Champion's cotton whites list 110–160. Print-flash-print when one pass doesn't block the shirt. Flash to a gel, not a cure. Cure the full film and keep reduction inside the label's limit. Champion's white plastisol printing guide sums it up: "The two main reasons white looks dull on dark shirts are: not enough ink laid down, or undercure."
Puff that won't rise, or rises under the flash
Won't rise: puff develops in the dryer, so a flat print is usually undercured or too thin. Champion's Puff label puts full cure at 320–330°F, where "the puff develops fully in the dryer," and calls for 86–110 mesh for maximum puff, with a thick stencil or multiple emulsion coats. Bold shapes rise better than hairlines. Too much heat causes the opposite problem: a scorched garment or collapsed puff.
Rises under the flash: the flash is too hot or too close. The label's fix: "If it puffs at the flash, lower the flash temperature or raise the flash height." More puff technique is in our fluorescent puff printing guide.
Water-based ink drying in the screen
Water-based ink dries as its water evaporates, and it will do that in the mesh if you let it. Ink that dries in the screen blocks fine detail and halftones first.
- Keep the screen flooded. Champion's Water-Based Fluorescent label: "Keep screens flooded to prevent ink drying in the mesh."
- Add retarder to extend open time. Champion's Water-Based Ink Retarder goes in at about 1–2% by weight, adjusted to your shop conditions and run length.
- Don't overload it. The retarder label warns, "Using too much retarder can slow cure and affect print durability."
- Keep containers sealed between jobs to prevent surface drying.
- Clean up with water while the ink is still wet.
Hot, dry shops are where water-based ink skins fastest, and the retarder's label lists them among its recommended uses.
Screen printing troubleshooting chart
A one-glance checklist for the press. Every fix assumes you're working inside the ranges on your ink's label.
| Symptom | Likely cause | Check, then fix |
|---|---|---|
| Cracks after a wash or stretch | Undercure; non-stretch ink on stretch fabric | Measure the ink film; add dwell time; use a stretch ink on stretch fabric |
| Ink washes out or fades | Undercure; thin deposit; over-reduction | Wash-test; check the reducer log; cure fully on the label's mesh |
| Pinholes | Stencil: dust, poor degreasing, underexposure | Check on a light table; degrease, recoat, run an exposure test, block out |
| Ghost or double image | Screen, platen or garment movement; ink under the screen | Tighten clamps; set off-contact; use pallet adhesive; wipe the underside |
| White turns pink on polyester | Dye migration | Check the first piece after 24 hours; lower the heat; low-bleed white; grey blocker |
| Dull or gray white | Thin deposit; undercure; over-reduction | Use the label's solids mesh; print-flash-print; cure fully |
| Puff stays flat | Undercure; thin deposit | Cure to the label's range; open mesh; thick stencil |
| Puff rises at the flash | Flash too hot or too close | Lower the flash temperature or raise the flash height |
| Water-based ink dries in the screen | Short open time; screen left unflooded | Keep it flooded; add retarder at about 1–2% by weight |
When to call Champion
If the checks above don't solve it, send us the details and we'll help you work through it. Include:
- the garment brand, style and fiber content
- the ink and series, from the label
- mesh count and stencil
- flash temperature and time
- dryer temperature, belt speed and the ink-film temperature you measured
- a photo of the problem, before and after washing if you have both
Talk to Champion about a print problem.
Shop the inks
Most fixes on this page come down to the right ink for the fabric and a full cure. Browse Champion plastisol inks, the Extreme 270° low-cure plastisol for heat-sensitive polyester, stretch plastisol for performance wear and the white plastisol inks. Printing water-based? See the water-based inks and retarder. For more guides, visit the Champion Learning Center.
Frequently asked questions
Why does my screen print crack after washing?
Most often the ink film was undercured: it gelled but never fully fused. Heavy deposits are the usual victims because their underside heats last. Measure the ink-film temperature against your ink's label, add dwell time before you add heat, and wash-test a sample. On stretch fabrics, use a stretch ink or additive, because a standard plastisol can crack when the fabric stretches.
Why is the ink washing out of my shirts?
Washout usually means undercure, a deposit too thin to hold up, or over-reduced ink. Check the ink-film temperature, not the dryer setting, and confirm it reaches the label's range. Print on the label's mesh so enough ink reaches the garment, and keep reducer inside the label limit; Champion's All Purpose label caps it at 5%. Wash-test before the run.
What causes pinholes in screen printing?
Pinholes come from the stencil: mesh that wasn't fully degreased, dust or lint on the mesh, film or glass, bubbles or uneven emulsion, underexposure, or a screen coated or exposed before it was dry. Degrease every screen, coat and dry in a clean, dark space, run an exposure test, and check each screen on a light table so you can block out pinholes before printing.
What causes ghosting in screen printing?
A ghost or double image means something moved or ink built up where it shouldn't. Check for loose clamps or frames, low mesh tension, too little off-contact and garments sliding on the platen. Wipe ink off the underside of the screen, and flash the underbase until it is dry to the touch so the next screen doesn't pick it up.
Why did my white print turn pink?
On polyester, a white that turns pink is dye migration: heat releases dye from the fabric into the ink. Lower the cure temperature with a low-cure ink, switch to a low-bleed white, and print a grey blocker underneath on dark or sublimated garments. Let prints cool before stacking, and check the first piece after 24 hours before running the order.